Marroko soul is a versatile and durable finish that originates from Morocco, and has gained popularity in Europe in the last decade. This lime-based plaster is hand-applied to create a smooth, satin finish that is both beautiful and functional. Its earthy, organic look brings warmth and character to any architectural space, making it an excellent choice for a range of interior and exterior applications. In addition, Tadelakt is easy to waterproof, making it ideal for use in damp environments such as bathrooms, shower walls, kitchens, and steam rooms.
100% NATURAL VERSION - GREEN LINE
Enjoy the same ease of application, durability and aesthetic qualities of the original product with its 100% natural version. Made with hydrated lime, selected marble powders, vegetable starches, cellulose, milk derivatives, and pozzolanic agents, this completely natural option eliminates all chemicals.
Document type Technical Data Sheet
Name MARROKO SOUL
Description Natural, lime-based material for decorative finishes on interior and exterior wall
surfaces. Naturally anti-mould and breathable. This lime-based plaster originates in
Marocco, where it is traditionally used in steam baths. It is appreciated for its durability
and satin, authentic appearance.
Composition Aged, slaked lime and selected marble powders.
Grain size 700 microns
Appearance Powder
Colour White, it can be tinted in any colour with lime-compatible colourants
Packaging 16 kg net polyethylene containers
Application By hand, with a steel trowel
Type of Surface New Wall Surface
Plaster: no priming necessary
Gypsum / Plasterboard / Medium Density: one coat of QUARTZ PRIMER
Old Wall Surface
Plaster: one coat of QUARTZ PRIMER
Fast drying / Limewash: brush down and apply one coat of QUARTZ PRIMER
Polished Lime: Abrade, brush down and apply one coat of QUARTZ PRIMER
Washable Paint: one coat of QUARTZ PRIMER
Dilution Each kg of MARROKO SOUL powder should be diluted with 360 ml of water. Therefore, in a
16 kg
Name MARROKO SOUL
Description Natural, lime-based material for decorative finishes on interior and exterior wall
surfaces. Naturally anti-mould and breathable. This lime-based plaster originates in
Marocco, where it is traditionally used in steam baths. It is appreciated for its durability
and satin, authentic appearance.
Composition Aged, slaked lime and selected marble powders.
Grain size 700 microns
Appearance Powder
Colour White, it can be tinted in any colour with lime-compatible colourants
Packaging 16 kg net polyethylene containers
Application By hand, with a steel trowel
Type of Surface New Wall Surface
Plaster: no priming necessary
Gypsum / Plasterboard / Medium Density: one coat of QUARTZ PRIMER
Old Wall Surface
Plaster: one coat of QUARTZ PRIMER
Fast drying / Limewash: brush down and apply one coat of QUARTZ PRIMER
Polished Lime: Abrade, brush down and apply one coat of QUARTZ PRIMER
Washable Paint: one coat of QUARTZ PRIMER
Dilution Each kg of MARROKO SOULpowder should be diluted with 360 ml of water. Therefore, in a
16 kg MARROKO SOUL tub, add 5.75 L of water.
Consumption 2 kg / sqm after three coats
Drying 3 hours at 20°C / 68°F to the touch
48 hours at 20°C / 68°F below the surface
180 days stable
Application temperatures min 5 max 30°C – R.U. < 85% ca
Coat Thickness 1.9 - 2 mm after three coats
VOC Classification EU Directive 2004/42/CE: EU limit value for this product (cat A/l – water-based
decorative effect coating): 200 g/l (2010). This product contains less than 1 g/l of VOC
Specific Weight 1.4 ± 0.2 (kg/l)
pH after 30 days 12.5 ± 0.50
Vapour Permeability SD ~ 0,04 m (DIN 52 615)
Flammability European Class of Reaction to Fire A1: non-combustible – no contribution to fire
Mould Resistance ASTM D 3274 – “Standard Test Method to evaluate the degree of surface
disfigurement of paint by microbial, fungal and algae growth.
Result: Front Panel 10/10/10 Back Panel 10/10/10 = no growth
Scrub Test Resistance ASTM D 2486-06 method A = was used: scrubbing fine sand + metallic brush for
10,000 cycles
TDS MARROKO SOUL October 23 2 of 5
Impact Test UNI EN ISO 6272-2-2006. 1 kg doming punch was dropped from different heights and
only at the height of 8 cm., it left a 5.5 mm. dent in the surface and a tiny crack
appeared around its circumference.
Pencil Hardness ASTM D3363- Pencil hardness 5H
Shore Hardness Norm ASTM 2240 average
Adhesion Norm UNI EN 13892-8 2004 average value = 2,0
Shelf life 24 months in sealed containers
Pot life 3 months on average, if stored correctly
Storage In original sealed packaging between 5° - 35°C in a dry, dark environment
Safety Norms Irritating. / Risk of serious damage to eyes. / Irritating to the skin. / Keep out of children.
/ Avoid contact with eyes. / In case of contact with eyes, clean immediately with water
without rubbing them, and consult a doctor. / Wear suitable gloves and eyes / face
protection. / In case of ingestion of the products, consult immediately a doctor showing
him the can or the label of the product. Danger labelling under directives 67/548/EEC
and 1999/45/EC nd following amendments and adjustments. The product must be
transported, used and stored according to current standards of hygiene and safety.
Disposal Product must be disposed of according to norms and regulations in force. Containers
must be sent for recycling. Follow directions on the packaging
Application Instructions WARNINGS
We recommend using materials from the same production batch for the same project.
If you must use different batches, we suggest mixing their material together to avoid
any slight variations in shading.
To ensure proper usage, dilution, and application of the products mentioned in these
pages, please consult the corresponding technical data sheets.
When preparing the surface and applying the materials, we advise using appropriate
tools and personal protective equipment (PPE).
During application and for the following 72 hours, protect the surfaces from sudden
temperature change, direct sun light and water. Don’t apply in temperatures below 8°C
or above 35°. During application make sure that the work area isn’t too damp to avoid
problems with application times.
Remember to have a strong light parallel to the wall and situated on only one of the
two sides of the wall you are working on (usually on the same side as other sources of
light such as windows). In this way the shadow of the trowel allows you to see the
actual state of the finish. Every so often, during the second and third coat, the light
should be moved so that the wall doesn’t dry out too much in one spot from the heat of
the lamp.
APPLICATION
Protection of the work area: Masking tape and protective material over the baseboards
and around windows and doors.
Marroko soul should be applied to plaster (rough or smooth, new or old). The perfect
TDS Marroko soul October 23 3 of 5
one is a rough plaster made with lime and sand. Already painted surfaces require a
thorough brushing down to remove dust and uneven parts.
Where necessary, use a brush or roller to apply a coat of QUARTZ PRIMER diluted
with water up to about 10% in volume to be used, ca. gr/m2 120 ÷ 150, or UNIVERAL
PRIMER diluted 1 to 8 with water. Mix the powder material with water as described
above. Tint it in the selected colour (you can use our Colouring System), mixing the
pigment very well until a homogeneous shade is obtained. Let the product rest for half
an hours before using it. You must apply at least two coats with a steel trowel.
1) FIRST COAT: use ca. 850-900 gr/m2. This coat is applied directly to the plaster
(background), taking care to apply it evenly to smooth out any imperfections in the
ground.
2) SECOND COAT : apply when the first coat is dry. Use ca. 1050-1300 g/sqm, taking
care that the surface is as smooth and groove-free as possible. Note that to get the
Moroccan effect you have to use till 1300 g per sqm, but most of the appliers use about
1000-1150 grams per sqm. Note that the application of a third very thin coat could help
if the wall absorbs too much.
3) Now it begins a work of pressing and smoothing with spatula and trowel. It has to be
done along with the drying process. If you press too much when the material is too wet
some bubbles will appear. For this part of the work you can also use a plastic spatula
with a well-prepared round edge. With the plastic spatula you have to press the
surface, until some of the water comes out, carrying some lime and the finer powders.
You need this “cream” to come out and fill the micro pores, which are produced by the
drying process. The same work you can get using a metallic trowel and a water spray
bottle. Be careful not to leave drops of water along the wall or they will create light
marks.Filling the micro-pores has the double purpose of creating more shine and to
make the surface waterproof. With a metallic and plastic trowel you can complete your
work. At the end it is suggested to use a plastic trowel and a cloth to make the surface
shinier.
A variation is the traditional Moroccan use of the stone for Marroko soul .
This is a rounded stone which has been cut in two equal parts. The flat part we get
from the cutting is made very smooth and shiny and the edge rounded and smoothed.
It is used with circular movements with the flat smooth surface against the surface of
the Marroko soul at the end of the work but when the material is still wet enough to
produce the cream of lime and fine powder that we described above. You can
understand that it is the proper time to use the stone because during the special
"burnishing" with the stone a typical sound is produced during the rubbing. With this
stone you can get a surface very waterproof since the micro porous can be fixed very
well. In addition, you get the surface with the special wavy effect a little like a brocade
fabric typical of the Moroccan bath.
EXTERIORS: For exterior applications there are some rules to respect and some
precautions to take. We remind you that carbonation, i.e. the process that takes place
through the absorption of atmospheric CO2, is completed in a few hours on the surface
but takes several days to take place in depth. It is therefore important that the
TDS Marroko soul October 23 4 of 5
application takes place in the certainty of the absence of heavy rains in the three
following days. It is also not recommended to apply it on walls that do not have at least
a small roof overhang. Penetrating rain could ruin the finish even after weeks as deep
carbonation is completed after more than a month. Avoid windy days, especially at high
temperatures, as well as the risk of frost in the 48 hours following application. In
external applications in hot climate conditions, it is also recommended to protect the
wall from the sun with shade cloths applied to the scaffolding. Lime-based products
must dry slowly to better fulfil their characteristics.
Finish Protection
(optional)
INTERIOR: BEESWAX / MINERAL WAX / HYDROCALCE / MARSEILLE SOAP /
MOROCCAN OLIVE OIL SOAP
EXTERIOR: HYDROCALCE
WET AREAS: PU1C
tub, add 5.75 L of water.
Consumption 2 kg / sqm after three coats
Drying 3 hours at 20°C / 68°F to the touch
48 hours at 20°C / 68°F below the surface
180 days stable
Application temperatures min 5 max 30°C – R.U. < 85% ca
Coat Thickness 1.9 - 2 mm after three coats
VOC Classification EU Directive 2004/42/CE: EU limit value for this product (cat A/l – water-based
decorative effect coating): 200 g/l (2010). This product contains less than 1 g/l of VOC
Specific Weight 1.4 ± 0.2 (kg/l)
pH after 30 days 12.5 ± 0.50
Vapour Permeability SD ~ 0,04 m (DIN 52 615)
Flammability European Class of Reaction to Fire A1: non-combustible – no contribution to fire
Mould Resistance ASTM D 3274 – “Standard Test Method to evaluate the degree of surface
disfigurement of paint by microbial, fungal and algae growth.
Result: Front Panel 10/10/10 Back Panel 10/10/10 = no growth
Scrub Test Resistance ASTM D 2486-06 method A = was used: scrubbing fine sand + metallic brush for
10,000 cycles
TDS MARROKO SOUL October 23 2 of 5
Impact Test UNI EN ISO 6272-2-2006. 1 kg doming punch was dropped from different heights and
only at the height of 8 cm., it left a 5.5 mm. dent in the surface and a tiny crack
appeared around its circumference.
Pencil Hardness ASTM D3363- Pencil hardness 5H
Shore Hardness Norm ASTM 2240 average
Adhesion Norm UNI EN 13892-8 2004 average value = 2,0
Shelf life 24 months in sealed containers
Pot life 3 months on average, if stored correctly
Storage In original sealed packaging between 5° - 35°C in a dry, dark environment
Safety Norms Irritating. / Risk of serious damage to eyes. / Irritating to the skin. / Keep out of children.
/ Avoid contact with eyes. / In case of contact with eyes, clean immediately with water
without rubbing them, and consult a doctor. / Wear suitable gloves and eyes / face
protection. / In case of ingestion of the products, consult immediately a doctor showing
him the can or the label of the product. Danger labelling under directives 67/548/EEC
and 1999/45/EC nd following amendments and adjustments. The product must be
transported, used and stored according to current standards of hygiene and safety.
Disposal Product must be disposed of according to norms and regulations in force. Containers
must be sent for recycling. Follow directions on the packaging
Application Instructions WARNINGS
We recommend using materials from the same production batch for the same project.
If you must use different batches, we suggest mixing their material together to avoid
any slight variations in shading.
To ensure proper usage, dilution, and application of the products mentioned in these
pages, please consult the corresponding technical data sheets.
When preparing the surface and applying the materials, we advise using appropriate
tools and personal protective equipment (PPE).
During application and for the following 72 hours, protect the surfaces from sudden
temperature change, direct sun light and water. Don’t apply in temperatures below 8°C
or above 35°. During application make sure that the work area isn’t too damp to avoid
problems with application times.
Remember to have a strong light parallel to the wall and situated on only one of the
two sides of the wall you are working on (usually on the same side as other sources of
light such as windows). In this way the shadow of the trowel allows you to see the
actual state of the finish. Every so often, during the second and third coat, the light
should be moved so that the wall doesn’t dry out too much in one spot from the heat of
the lamp.
APPLICATION
Protection of the work area: Masking tape and protective material over the baseboards
and around windows and doors.
Marroko soul should be applied to plaster (rough or smooth, new or old). The perfect
TDS Marroko soul October 23 3 of 5
one is a rough plaster made with lime and sand. Already painted surfaces require a
thorough brushing down to remove dust and uneven parts.
Where necessary, use a brush or roller to apply a coat of QUARTZ PRIMER diluted
with water up to about 10% in volume to be used, ca. gr/m2 120 ÷ 150, or UNIVERAL
PRIMER diluted 1 to 8 with water. Mix the powder material with water as described
above. Tint it in the selected colour (you can use our Colouring System), mixing the
pigment very well until a homogeneous shade is obtained. Let the product rest for half
an hours before using it. You must apply at least two coats with a steel trowel.
1) FIRST COAT: use ca. 850-900 gr/m2. This coat is applied directly to the plaster
(background), taking care to apply it evenly to smooth out any imperfections in the
ground.
2 ) SECOND COAT : apply when the first coat is dry. Use ca. 1050-1300 g/sqm, taking
care that the surface is as smooth and groove-free as possible. Note that to get the
Moroccan effect you have to use till 1300 g per sqm, but most of the appliers use about
1000-1150 grams per sqm. Note that the application of a third very thin coat could help
if the wall absorbs too much.
3) Now it begins a work of pressing and smoothing with spatula and trowel. It has to be
done along with the drying process. If you press too much when the material is too wet
some bubbles will appear. For this part of the work you can also use a plastic spatula
with a well-prepared round edge. With the plastic spatula you have to press the
surface, until some of the water comes out, carrying some lime and the finer powders.
You need this “cream” to come out and fill the micro pores, which are produced by the
drying process. The same work you can get using a metallic trowel and a water spray
bottle. Be careful not to leave drops of water along the wall or they will create light
marks.Filling the micro-pores has the double purpose of creating more shine and to
make the surface waterproof. With a metallic and plastic trowel you can complete your
work. At the end it is suggested to use a plastic trowel and a cloth to make the surface
shinier.
A variation is the traditional Moroccan use of the stone for Marroko soul .
This is a rounded stone which has been cut in two equal parts. The flat part we get
from the cutting is made very smooth and shiny and the edge rounded and smoothed.
It is used with circular movements with the flat smooth surface against the surface of
the Marroko soul at the end of the work but when the material is still wet enough to
produce the cream of lime and fine powder that we described above. You can
understand that it is the proper time to use the stone because during the special
"burnishing" with the stone a typical sound is produced during the rubbing. With this
stone you can get a surface very waterproof since the micro porous can be fixed very
well. In addition, you get the surface with the special wavy effect a little like a brocade
fabric typical of the Moroccan bath.
EXTERIORS: For exterior applications there are some rules to respect and some
precautions to take. We remind you that carbonation, i.e. the process that takes place
through the absorption of atmospheric CO2, is completed in a few hours on the surface
but takes several days to take place in depth. It is therefore important that the
TDS Marroko soul October 23 4 of 5
application takes place in the certainty of the absence of heavy rains in the three
following days. It is also not recommended to apply it on walls that do not have at least
a small roof overhang. Penetrating rain could ruin the finish even after weeks as deep
carbonation is completed after more than a month. Avoid windy days, especially at high
temperatures, as well as the risk of frost in the 48 hours following application. In
external applications in hot climate conditions, it is also recommended to protect the
wall from the sun with shade cloths applied to the scaffolding. Lime-based products
must dry slowly to better fulfil their characteristics.
Finish Protection
(optional)
INTERIOR: BEESWAX / MINERAL WAX / HYDROCALCE / MARSEILLE SOAP /
MOROCCAN OLIVE OIL SOAP
EXTERIOR: HYDROCALCE
WET AREAS: PU1C
We have drawn up the material presented above to the best of our technical and experiential knowledge. Nevertheless,
our suggestions and recommendations are not guaranteed. All responsibility for the obtained results lies solely with the
method and conditions adopted for the application of the product. Such indications constitute valid support for verifying
the product's suitability for the specific case. We reserve the right to make modifications to the present information